Biodegradable synthetic polymers for biomedical and tissue engineering applications: tailoring degradation kinetics with tissue regeneration timeline
Open accessThe DOI matches its Crossref record; 142 of the 142 references it cites were found in a registry or an index; none of the 119 sources its claims cite is checked for support yet.
Abstract
The adoption of biodegradable synthetic polymers in biomedical and tissue engineering becomes a focal point, offering alternative solutions to organ transplantation and conventional permanent restoration. The key principle in developing scaffold-based for physiological implantation is the synchronisation of polymer’s degradation kinetics with the regeneration timeline of host tissues. Different implantation lesions exhibit vastly different healing durations, ranging from a few weeks to several months or years. A mismatch timeline can be detrimental where premature degradation will remove the physical framework needed for cell integration, whereas overly slow degradation will restrict spaces for new tissue growth. This review study provides a comprehensive discussion on the degradation mechanisms of biodegradable synthetic polymers in physiological environments. Four widely studied polymers—polylactic acid (PLA), polyvinyl alcohol (PVA), polycaprolactone (PCL), and polyurethane (PU)—were reviewed in depth on the degradation mechanisms and influencing factors. Scientific experimental data from the previous studies were summarised, including degradation percentage, experimental conditions, degradation timeline, and estimated complete degradation period. Specifically, four degradation mechanisms are associated with the degradation of synthetic polymers in physiological environments including chemical hydrolysis, enzymatic-mediated metabolism, oxidative degradation, and pH-dependent degradation. Each of the mechanisms may act independently or synergistically under different biological conditions. The degradation of polymers is accordingly influenced by the chemical structures, fabrication routes, degradation pathways, and physicochemical factors. These data are correlated with their optimal use in biomedical and TE applications for fast regenerating tissues to slow-healing or load-bearing structures. Comprehensively, PVA is aligned well with short-to-intermediate healing tissues such as the skin and the cornea due to its high degradation capability, while PLA, PCL, and PU that degrade from weeks to years are suitable for mediate-healing soft tissues to long-term implantations such as load-bearing bone, cartilage, ligament, neural, and vascular implantations. By aligning polymer degradation profiles with the biological timelines of tissue regeneration, this review provides a translational framework for synthetic polymer selection to enable optimum scaffold’s functionalities and clinical outcomes.
Overview
CoChat Summary
## TL;DR
This review argues that biodegradable synthetic polymers for tissue engineering should be chosen and tuned so their degradation matches the regeneration timeline of the target tissue. It focuses on PLA, PVA, PCL, and PU, summarizing their degradation mechanisms, the factors that alter degradation, and how those profiles fit different biomedical applications.
## Key findings
- The paper states that different tissues regenerate on different timelines: skin can remodel in “as minimum as 2 weeks,” bone often needs “6–12 weeks,” and cartilage, ligament, vascular, and neural tissues can take “several months to over a year.”
- It identifies four main degradation mechanisms relevant to synthetic polymers in tissue engineering: chemical hydrolysis, enzymatic-mediated reaction, oxidative degradation, and pH-dependent degradation.
- For PLA, the review reports degradation examples ranging from very low loss to substantial loss depending on formulation and environment, including “0–1%” over 4 weeks for 3D-printed PLA in PBS, “20.10%” weight loss for PLA-casted scaffolds in PBS, and about “10%” weight loss at 20 weeks.
- For PVA, degradation ranged from “~90–100% after 10 days” for electrospun nanofibres in PBS to “~8–15% over 4 weeks” for freeze-thawed and freeze-dried scaffolds; the paper notes PVA is used mostly for skin TE that needs “days to weeks” of degradation.
- For PCL, the paper reports very slow degradation in many cases, including “0.6% in 28 days” for cylindrical filaments and “4–5% over” 28 weeks for electrospun nanofibres; it states PCL is widely used for bone TE.
- For PU, the review reports degradation examples from “2.7–5.0% at 12 months” for cast films to “80% over a span of three years” for foams, with the paper emphasizing its use in vascular and neural TE applications.
## Methods
- This is a narrative review article, not an original experimental study.
- It synthesizes published literature on biodegradable synthetic polymers, especially PLA, PVA, PCL, and PU, and compares reported degradation behaviors across studies.
- The main analysis is interpretive: it aligns polymer degradation kinetics with tissue regeneration timelines and discusses how structure, crystallinity, porosity, hydrophilicity, and surface chemistry affect degradation.
## Limitations
- The paper does not state a formal study limitation section; this is not stated in the paper.
- It explicitly says it focuses on selected biodegradable polymers and that “future studies” should extend the concepts to additional synthetic polymeric systems beyond the review’s scope.
- Evident from the text: the evidence base is heterogeneous across many cited studies with different materials, assays, media, and time points, so the comparisons are qualitative rather than a controlled head-to-head analysis.
Model-written summary. Check it against the paper before relying on it.
Integrity signals
Registry
Cites
Statistics
Figures



![Fig. 4 Clearance routes for the degradation by-products of PLA, PVA, PCL, and PU that involve various functional organs such as kidney, lung, liver, and skin (created with NotebookLM) [54–56, 78, 79, 93, 103, 143, 144]](https://figures.cochat.ai/paper-figures/6e894ca601a247d6a5bb7ec7a14fc484/biodegradable-synthetic-polymers-for-biomedical-and-tissue-engineering-figure-4.jpg)
Verification
Claims the paper makes
0 Valid · 4 Not valid · 102 Not checked · 53 Own results and interpretations
None of the sources cited for this claim have been checked yet.
In the paper
“Another important trait to be emphasised in polymer selection is the biodegradable timeline where different types of tissue require different timelines for complete remodelling/regeneration in the human body.”
What the sources say
- Not checked yetcites [28] Qin J, Chen F, Wu P, Sun G. Recent advances in bioengineered scaffolds for cutaneous wound healing. Front Bioeng Biotechnol. 2022;1(10):841583. https://doi.org/10.3389/fbioe.2022.841583. source
- Not checked yetcites [29] Puodziunas V. Tissue Regeneration Process for Healing Injuries. Regenerative Healing: How the Body Repairs Tissue Damage. 2025. https://watersedgemedicalclinic.com/tissue-regeneration-process-for-healing-injuries. Accessed 26 Nov 2025
plainstates an association- Asserted: passes — The authors put it forward as true.
- Checkable: passes — It can be checked against evidence.
- Load-bearing: passes — The paper’s conclusions depend on it.
- Based: passes — The paper gives a reason why it holds.
In the paper
“Biodegradable scaffolds possess an ability to degrade simultaneously in the surrounding aqueous environment without the need for surgical removal [ 18 ].”
What the sources say
- Not checked yetcites [18] Haider A, Haider S, Kummara MR, Kamal T, Alghyamah A-A, Iftikhar FJ, et al. Advances in the scaffolds fabrication techniques using biocompatible polymers and their biomedical application: a technical and statistical review. J Saudi Chem Soc. 2020;24(2):186–215. https://doi.org/10.1016/j.jscs.2020.01.002. source
plain- Asserted: passes — The authors put it forward as true.
- Checkable: passes — It can be checked against evidence.
- Load-bearing: passes — The paper’s conclusions depend on it.
- Based: passes — The paper gives a reason why it holds.
In the paper
“In controlling the biodegradation of synthetic polymers, unstable chemical linkages such as amides, anhydrides, labile esters, orthoesters, etc., can be incorporated in polymer backbones as these bonds are prone to undergo common hydrolytic or enzymatic degradation mechanisms [ 34 ].”
What the sources say
- Not checked yetcites [34] Garcia-Garcia A, Muñana-González S, Lanceros-Mendez S, Ruiz-Rubio L, Alvarez LP, Vilas-Vilela JL. Biodegradable natural hydrogels for TE, controlled release, and soil remediation. Polymers. 2024;16(18):2599. https://doi.org/10.3390/polym16182599. source
plainstates a cause- Asserted: passes — The authors put it forward as true.
- Checkable: passes — It can be checked against evidence.
- Load-bearing: passes — The paper’s conclusions depend on it.
- Based: passes — The paper gives a reason why it holds.
None of the sources cited for this claim have been checked yet.
In the paper
“The kinetics of bond cleavage are directly correlated to the type of bonds present in a particular polymeric chain [ 35 , 36 ].”
What the sources say
- Not checked yetcites [35] Ewii UE, Onugwu AL, Nwokpor VC, Akpaso I, Ogbulie TE, Aharanwa B, et al. Novel drug delivery systems: insight into self-powered and nano-enabled drug delivery systems. Nano TransMed. 2024;3:100042. https://doi.org/10.1016/j.ntm.2024.100042. source
- Not checked yetcites [36] Grivet-Brancot A, Boffito M, Ciardelli G. Use of polyesters in fused deposition modeling for biomedical applications. Macromol Biosci. 2022;22(10):e2200039. https://doi.org/10.1002/mabi.202200039. source
plainstates an association- Asserted: passes — The authors put it forward as true.
- Checkable: passes — It can be checked against evidence.
- Load-bearing: unclear — It is unclear whether the paper’s conclusions depend on it.
- Based: passes — The paper gives a reason why it holds.
None of the sources cited for this claim have been checked yet.
In the paper
“To alleviate these limitations, tissue engineering (TE) in combination with biomaterials is known to be the most reliable alternative to replace the procedure of organ transplantation in supporting successful tissue regeneration [ 10 , 11 ].”
What the sources say
- Not checked yetcites [10] Han F, Wang J, Ding L, Hu Y, Li W, Yuan Z, et al. TE and regenerative medicine: achievements, future, and sustainability in Asia. Front Bioeng Biotechnol. 2020;8:83. https://doi.org/10.3389/fbioe.2020.00083. source
- Not checked yetcites [11] Liu S, Yu J-M, Gan Y-C, Qiu X-Z, Gao ZC, Wang H, et al. Biomimetic natural biomaterials for TE and regenerative medicine: New biosynthesis methods, recent advances, and emerging applications. Military Med Res. 2023. https://doi.org/10.1186/s40779-023-00448-w. source
boostedstates a cause- Asserted: passes — The authors put it forward as true.
- Checkable: passes — It can be checked against evidence.
- Load-bearing: unclear — It is unclear whether the paper’s conclusions depend on it.
- Based: passes — The paper gives a reason why it holds.
75 more claims
Create a free account to see all 159 claims and to verify the 119 references still open.
- Probably not a substantial claim. 40
- It may state two separate claims as one. 47
- The quote only partly states this claim. 3
Self-check
Percentages, sums and reported differences re-computed from the paper’s own numbers.
This check didn’t finish.
Citations
Cites
Microbial and Enzymatic Degradation of Synthetic Plastics
Mohanan, N., Montazer, Z., Sharma, P. K., & Levin, D. B. (2020) · Frontiers in Microbiology · doi:10.3389/fmicb.2020.580709 · Cited by 1,122 · cited 2×
“Further degradation of urethane and urea units will direct into the release of free polyamines that depends on the initial composition of monomers [41].”
A Comparative Review of Natural and Synthetic Biopolymer Composite Scaffolds
Reddy, M. S. B., Ponnamma, D., Choudhary, R., & Sadasivuni, K. K. (2021) · Polymers · doi:10.3390/polym13071105 · Cited by 1,104 · cited 1×
“Polymeric biodegradable materials can be classified into natural and synthetic polymers [15, 16].”
Bharadwaz, A., & Jayasuriya, A. C. (2020) · Materials Science and Engineering: C · doi:10.1016/j.msec.2020.110698 · Cited by 738
Zaaba, N. F., & Jaafar, M. (2020) · Polymer Engineering & Science · doi:10.1002/pen.25511 · Cited by 683 · cited 1×
“…by the amount of water penetrating amorphous regions; (3) the autocatalytic acceleration of hydrolysis caused by carboxylic end-group formation; and (4) the generation of hydrophilic degradation by-products, which ultimately results in substantial weight loss and dissolution of polymer matrix [57].”
Natural and Synthetic Polymers for Biomedical and Environmental Applications
Satchanska, G., Davidova, S., & Petrov, P. D. (2024) · Polymers · doi:10.3390/polym16081159 · Cited by 585 · cited 2×
“In addition, surface attributes including wettability, surface charge, polarity, surface roughness, and available chemical moieties on the surface exhibit important roles in aligning degradation targets [22].”
Poly(vinyl alcohol): review of its promising applications and insights into biodegradation
Ben Halima, N. (2016) · RSC Advances · doi:10.1039/c6ra05742j · Cited by 440 · cited 1×
“Polyvinyl alcohol is also degraded through a chemical hydrolysis mechanism at a relatively slow rate compared to an enzymatic-mediation reaction due to the stability of its carbon–carbon backbone and the absence of easily hydrolysable linkages such as esters or amides [79].”
Biodegradable materials for bone defect repair
Wei, S., Ma, J.-X., Xu, L., Gu, X.-S., & Ma, X.-L. (2020) · Military Medical Research · doi:10.1186/s40779-020-00280-6 · Cited by 406 · cited 1×
“Despite the biofunctional and bioactivity of natural-based polymers, synthetic polymers are worth expanding research, owing to their stability, mechanical integrity, uniform framework, sustainable degradation, versatile processing modification, and feasible resources [17].”
Khouri, N. G., Bahú, J. O., Blanco-Llamero, C., Severino, P., Concha, V. O. C., & Souto, E. B. (2024) · Journal of Molecular Structure · doi:10.1016/j.molstruc.2024.138243 · Cited by 403 · cited 2×
“However, hydrolysis normally encompasses complex reaction pathways since several different cleavage reactions can happen side by side [52].”
Design Challenges in Polymeric Scaffolds for Tissue Engineering
Echeverria Molina, M. I., Malollari, K. G., & Komvopoulos, K. (2021) · Frontiers in Bioengineering and Biotechnology · doi:10.3389/fbioe.2021.617141 · Cited by 397
Arif, Z. U., Khalid, M. Y., Noroozi, R., Sadeghianmaryan, A., Jalalvand, M., & Hossain, M. (2022) · International Journal of Biological Macromolecules · doi:10.1016/j.ijbiomac.2022.07.140 · Cited by 395
Mozafari, M., Moztarzadeh, Jalali, Alhosseini, N., Asgari, Dodel, Samadikuchaksaraei, & Kargozar (2012) · International Journal of Nanomedicine · doi:10.2147/ijn.s25376 · Cited by 370
Tissue Engineering and Regenerative Medicine: Achievements, Future, and Sustainability in Asia
Han, F., Wang, J., Ding, L., Hu, Y., Li, W., Yuan, Z., Guo, Q., Zhu, C., Yu, L., Wang, H., et al. (2020) · Frontiers in Bioengineering and Biotechnology · doi:10.3389/fbioe.2020.00083 · Cited by 357
Liu, S., Yu, J.-M., Gan, Y.-C., Qiu, X.-Z., Gao, Z.-C., Wang, H., Chen, S.-X., Xiong, Y., Liu, G.-H., Lin, S.-E., et al. (2023) · Military Medical Research · doi:10.1186/s40779-023-00448-w · Cited by 357
Liang, X., Zhong, H.-J., Ding, H., Yu, B., Ma, X., Liu, X., Chong, C.-M., & He, J. (2024) · Polymers · doi:10.3390/polym16192755 · Cited by 332 · cited 1×
“These properties drive its use in biomedical and TE applications, enabling the fabrication of wound dressings, contact lenses, artificial cartilages, and tissue scaffolds [74].”
A review on PLA-based biodegradable materials for biomedical applications
Hussain, M., Khan, S. M., Shafiq, M., & Abbas, N. (2024) · Giant · doi:10.1016/j.giant.2024.100261 · Cited by 326 · cited 2×
“The degradation occurs mainly through autocatalysis, end chain, random chain scission, surface erosion, and bulk erosion [55].”
Electrospun Polycaprolactone (PCL) Degradation: An In Vitro and In Vivo Study
Dias, J. R., Sousa, A., Augusto, A., Bártolo, P. J., & Granja, P. L. (2022) · Polymers · doi:10.3390/polym14163397 · Cited by 293 · cited 1×
“Its promising attributes such as availability, stable structure, easy processing, superior mechanical properties, long-term degradation profile, and biocompatibility cause this polymer to be demanded for TE and drug delivery applications [95, 96].”
Scaffold degradation in bone tissue engineering: An overview
Tajvar, S., Hadjizadeh, A., & Samandari, S. S. (2023) · International Biodeterioration & Biodegradation · doi:10.1016/j.ibiod.2023.105599 · Cited by 291
Vlachopoulos, A., Karlioti, G., Balla, E., Daniilidis, V., Kalamas, T., Stefanidou, M., Bikiaris, N. D., Christodoulou, E., Koumentakou, I., Karavas, E., et al. (2022) · Pharmaceutics · doi:10.3390/pharmaceutics14020359 · Cited by 277 · cited 2×
“These enantiomers can form three different types of PLA molecules; L-lactide (PLLA), D-lactide (PDLA), and D, L-lactide (PDLLA); with distinct features through controlled polymerisation processes [50].”
Biodegradation of Biodegradable Polymers in Mesophilic Aerobic Environments
Bher, A., Mayekar, P. C., Auras, R. A., & Schvezov, C. E. (2022) · International Journal of Molecular Sciences · doi:10.3390/ijms232012165 · Cited by 254 · cited 2×
“This reaction is susceptible to either bulk polymers through bulk erosion or polymer surfaces through surface erosion that can be identified through mathematical modelling equations [40].”
Recent advances in responsive hydrogels for diabetic wound healing
Zhang, S., Ge, G., Qin, Y., Li, W., Dong, J., Mei, J., Ma, R., Zhang, X., Bai, J., Zhu, C., et al. (2023) · Materials Today Bio · doi:10.1016/j.mtbio.2022.100508 · Cited by 232 · cited 1×
“In the acidic environments of infected lesions, inflamed tissues, ischaemic or tumour tissues, polymers containing acid-or base-linkages will be easily degraded [47].”
Recent advances in oxidative degradation of plastics
Oh, S., & Stache, E. E. (2024) · Chemical Society Reviews · doi:10.1039/d4cs00407h · Cited by 227
Feng, P., Jia, J., Liu, M., Peng, S., Zhao, Z., & Shuai, C. (2021) · Materials & Design · doi:10.1016/j.matdes.2021.110066 · Cited by 224 · cited 1×
“The products are further metabolised inside the human body to be excreted [54].”
Production and Application of Biomaterials Based on Polyvinyl alcohol (PVA) as Wound Dressing
Jin, S. G. (2022) · Chemistry – An Asian Journal · doi:10.1002/asia.202200595 · Cited by 218
Biopolymer-based composites for tissue engineering applications: A basis for future opportunities
Zarrintaj, P., Seidi, F., Youssefi Azarfam, M., Khodadadi Yazdi, M., Erfani, A., Barani, M., Chauhan, N. P. S., Rabiee, N., Kuang, T., Kucinska-Lipka, J., et al. (2023) · Composites Part B: Engineering · doi:10.1016/j.compositesb.2023.110701 · Cited by 215
Poly lactic acid (PLA) polymers: from properties to biomedical applications
Ebrahimi, F., & Ramezani Dana, H. (2022) · International Journal of Polymeric Materials and Polymeric Biomaterials · doi:10.1080/00914037.2021.1944140 · Cited by 214 · cited 1×
“The competence of low molecular weight PLA to degrade under physiological conditions along with its non-toxicity and biocompatible nature make it a suitable candidate for biomedical applications [50, 51].”
Construction methods and biomedical applications of PVA-based hydrogels
Zhong, Y., Lin, Q., Yu, H., Shao, L., Cui, X., Pang, Q., Zhu, Y., & Hou, R. (2024) · Frontiers in Chemistry · doi:10.3389/fchem.2024.1376799 · Cited by 207 · cited 1×
“Due to the presence of abundant hydroxyl groups, PVA is known to be water-soluble, making this polymer in-match with the hydrophilic moieties of most drugs, bioactive materials, biomolecules, and herbs, thus allowing the formation of a homogenous blending composition [73].”
Magnin, A., Pollet, E., Perrin, R., Ullmann, C., Persillon, C., Phalip, V., & Avérous, L. (2019) · Waste Management · doi:10.1016/j.wasman.2018.12.024 · Cited by 199 · cited 1×
“The hard segments, typically composed of urethane or urea groups formed from biocompatible diisocyanates, are more resistant but can also be degraded slowly under prolonged enzymatic exposure [127, 128].”
Haider, A., Haider, S., Rao Kummara, M., Kamal, T., Alghyamah, A.-A. A., Jan Iftikhar, F., Bano, B., Khan, N., Amjid Afridi, M., Soo Han, S., et al. (2020) · Journal of Saudi Chemical Society · doi:10.1016/j.jscs.2020.01.002 · Cited by 188 · cited 1×
“Biodegradable scaffolds possess an ability to degrade simultaneously in the surrounding aqueous environment without the need for surgical removal [18].”
Naser, A. Z., Deiab, I., Defersha, F., & Yang, S. (2021) · Polymers · doi:10.3390/polym13234271 · Cited by 180 · cited 1×
“The hydrolytic cleavage in amorphous PLA regions is significantly facile as compared to the crystalline region where water diffuses linearly into the amorphous regions [60].”
Anjum, S., Rahman, F., Pandey, P. K., Arya, D. K., Alam, M., Rajinikanth, P. S., & Ao, Q. (2022) · International Journal of Molecular Sciences · doi:10.3390/ijms23169206 · Cited by 175
Biodegradable Natural Hydrogels for Tissue Engineering, Controlled Release, and Soil Remediation
García-García, A., Muñana-González, S., Lanceros-Méndez, S., Ruiz‐Rubio, L., Pérez‐Álvarez, L., & Vilas‐Vilela, J. L. (2024) · Polymers · doi:10.3390/polym16182599 · Cited by 175
Amino acid metabolism, transport and signalling in the liver revisited
Paulusma, C. C., Lamers, W. H., Broer, S., & van de Graaf, S. F. J. (2022) · Biochemical Pharmacology · doi:10.1016/j.bcp.2022.115074 · Cited by 172 · cited 1×
“Larger and partially hydrophobic or reactive breakdown by-products are taken up by the liver for detoxification, conjugation, and bile excretion [144].”
Long-Term Infectious Complications of Kidney Transplantation
Agrawal, A., Ison, M. G., & Danziger-Isakov, L. (2022) · Clinical Journal of the American Society of Nephrology · doi:10.2215/cjn.15971020 · Cited by 165 · cited 1×
“Furthermore, these procedures are accompanied by common post-operative issues such as tissue toxicity, immune rejection, inflammation, and bacterial infection [7–9].”
Branson, Y., Söltl, S., Buchmann, C., Wei, R., Schaffert, L., Badenhorst, C. P. S., Reisky, L., Jäger, G., & Bornscheuer, U. T. (2023) · Angewandte Chemie International Edition · doi:10.1002/anie.202216220 · Cited by 165 · cited 1×
“The enzymatic degradation of PU occurs through the action of biological enzymes that cleave specific bonds within the polymer structure, particularly ester, urethane (car-bamate), and sometimes urea linkages [125].”
Degradation Behavior of Polymers Used as Coating Materials for Drug Delivery—A Basic Review
Visan, A. I., Popescu-Pelin, G., & Socol, G. (2021) · Polymers · doi:10.3390/polym13081272 · Cited by 161 · cited 1×
“…cells, NGF nerve growth factor, PDGF platelet-derived growth factor, PNS peripheral nervous system, TGF-β transforming growth factor-beta, VEGF vascular growth factor act independently or synergistically, depending on the polymer type, chemical structure, and environmental conditions [32].”
Poly(lactic acid)-Based Electrospun Fibrous Structures for Biomedical Applications
Maleki, H., Azimi, B., Ismaeilimoghadam, S., & Danti, S. (2022) · Applied Sciences · doi:10.3390/app12063192 · Cited by 152 · cited 1×
“The drop in pH gradient will automatically and simultaneously induce more material’s degradation that will be converted into the common PLA by-products of H 2 O and CO 2 [56].”
Recent Advances in Polycaprolactones for Anticancer Drug Delivery
Bhadran, A., Shah, T. V., Babanyinah, G. K., Polara, H., Taslimy, S., Biewer, M. C., & Stefan, M. C. (2023) · Pharmaceutics · doi:10.3390/pharmaceutics15071977 · Cited by 149 · cited 2×
“The mild reaction conditions and scalability of this synthesis process make PCL an attractive option for industrial-scale production and biomedical applications that require high-purity and customisable polymeric materials [100].”
Backes, E. H., Harb, S. V., Beatrice, C. A. G., Shimomura, K. M. B., Passador, F. R., Costa, L. C., & Pessan, L. A. (2022) · Journal of Biomedical Materials Research Part B: Applied Biomaterials · doi:10.1002/jbm.b.34997 · Cited by 142
Polymer degradation: a short review
Vohlídal, J. (2021) · Chemistry Teacher International · doi:10.1515/cti-2020-0015 · Cited by 140 · cited 1×
“The ROS induce chain scission, crosslinking, or backbone oxidation, which result in the formation of carbonyl-containing degradation products such as aldehydes, ketones, and carboxylic acids [131, 132].”
Patil, P., Russo, K. A., McCune, J. T., Pollins, A. C., Cottam, M. A., Dollinger, B. R., DeJulius, C. R., Gupta, M. K., D’Arcy, R., Colazo, J. M., et al. (2022) · Science Translational Medicine · doi:10.1126/scitranslmed.abm6586 · Cited by 140 · cited 1×
“The functional groups in PU that are most susceptible to oxidative attack include ether, urethane, and aromatic segments [129, 130].”
Shiva, S. M., G, A. P. R., Bajaj, G., John, A. E., Sharan Chandran, M., Kumar, V. V., & Ramakrishna, S. (2023) · Journal of Materials Science Materials in Medicine · doi:10.1007/s10856-023-06765-9 · Cited by 136 · cited 1×
“The ester linkages are susceptible to being dissociated into smaller fragments, eventually producing safe degradation products of carbon dioxide, water, and small organic molecules [49].”
Rosato, A., Romano, A., Totaro, G., Celli, A., Fava, F., Zanaroli, G., & Sisti, L. (2022) · Polymers · doi:10.3390/polym14091850 · Cited by 134 · cited 1×
“For bulkier scaffolds such as PCL bone bricks, the initial pore size of 333–389 μm and porosity above 50% enabled a moderate 5.07% degradation within 5 days [110].”
InfluentialStructural engineering of polyurethanes for biomedical applications
Wang, H., Li, T., Li, J. X., Zhao, R., Ding, A., & Xu, F. (2024) · Progress in Polymer Science · doi:10.1016/j.progpolymsci.2024.101803 · Cited by 134 · cited 1×
“This polymer has superior mechanical properties compared to other synthetic polymers and possesses long-term degradation stability [120].”
Recent Advances in Bioengineered Scaffolds for Cutaneous Wound Healing
Qin, J., Chen, F., Wu, P., & Sun, G. (2022) · Frontiers in Bioengineering and Biotechnology · doi:10.3389/fbioe.2022.841583 · Cited by 132 · cited 2×
“Generally, some tissues are regenerated in a few weeks and others may reach more than a year for complete regeneration, depending upon the age and health history of an individual [28, 29].”
Developments of polyurethane in biomedical applications: A review
Cui, M., Chai, Z., Lu, Y., Zhu, J., & Chen, J. (2023) · Resources Chemicals and Materials · doi:10.1016/j.recm.2023.07.004 · Cited by 127 · cited 1×
“Most PUs are classified as thermosetting polymers that do not melt when heated while thermoplastic PUs are also available in the market [118, 119].”
Progress of gelatin-based 3D approaches for bone regeneration
Echave, M. C., Sánchez, P., Pedraz, J. L., & Orive, G. (2017) · Journal of Drug Delivery Science and Technology · doi:10.1016/j.jddst.2017.04.012 · Cited by 123 · cited 1×
“…and development of polymeric biodegradable materials that are defined as a three-dimensional (3D) framework capable of being used as a template to induce cell growth and support tissue regeneration while averting inflammation and restoring the normal operation of damaged tissues and organs [12–14].”
Designing of gradient scaffolds and their applications in tissue regeneration
Pattnaik, A., Sanket, A. S., Pradhan, S., Sahoo, R., Das, S., Pany, S., Douglas, T., Dandela, R., Liu, Q., Rajadas, J., et al. (2023) · Biomaterials · doi:10.1016/j.biomaterials.2023.122078 · Cited by 123 · cited 1×
“The compliance between the polymeric scaffold and adjacent cells is significantly influenced by the intrinsic properties of the scaffold’s material [26].”
Current advances in polyurethane biodegradation
Jin, X., Dong, J., Guo, X., Ding, M., Bao, R., & Luo, Y. (2022) · Polymer International · doi:10.1002/pi.6360 · Cited by 122 · cited 2×
“In primary hydrolytic degradation, ester bonds are hydrolysed into subsequence degradation products of α-hydroxy, urethane, and urea units with terminal acid groups [124].”
Sikdar, P. P., Dip, T. M., Dhar, A. K., Bhattacharjee, M., Hoque, M. S., & Ali, S. B. (2022) · Journal of Applied Polymer Science · doi:10.1002/app.52832 · Cited by 122 · cited 1×
“It is composed of soft and hard segments where its structure can be chemically synthesised to meet the specific requirements of various tissues, ranging from soft (e.g., skin, cardiac) to load-bearing (e.g., bone) applications [119, 121].”
Fathi, A., Khanmohammadi, M., Goodarzi, A., Foroutani, L., Mobarakeh, Z. T., Saremi, J., Arabpour, Z., & Ai, J. (2020) · Journal of Biological Engineering · doi:10.1186/s13036-020-00249-y · Cited by 121 · cited 1×
“[86], electrospun PVA fibres with diameter of 842 ± 205 nm, pore size of 1.33 ± 0.49 μm, and porosity percentage of 74 ± 3.9% showed moderate degradation (~ 20–30”
InfluentialBolívar‐Monsalve, E. J., Álvarez, M. M., Hosseini, S., Espinosa-Hernandez, M. A., Ceballos‐González, C. F., Sánchez‐Domínguez, M., Shin, S. R., Çeçen, B., Hassan, S., Maio, E. D., et al. (2021) · Materials Advances · doi:10.1039/d1ma00092f · Cited by 120
Biodegradable polycaprolactone (PCL) based polymer and composites
Archer, E., Torretti, M., & Madbouly, S. (2023) · Physical Sciences Reviews · doi:10.1515/psr-2020-0074 · Cited by 119
The influence of the functional end groups on the properties of polylactide-based materials
Kost, B., Basko, M., Bednarek, M., Socka, M., Kopka, B., Łapienis, G., Biela, T., Kubisa, P., & Brzeziński, M. (2022) · Progress in Polymer Science · doi:10.1016/j.progpolymsci.2022.101556 · Cited by 114 · cited 1×
“In chemical hydrolysis, susceptible moieties in a polymeric structure undergo autocatalytic scission upon interaction with water molecules and fragment into smaller oligomer and monomeric units without any enzymatic aid [39].”
Ahmad, A., Banat, F., Alsafar, H., & Hasan, S. (2022) · Biomass Conversion and Biorefinery · doi:10.1007/s13399-022-02581-3 · Cited by 113 · cited 1×
“It can be tuned by altering the stereochemistry, chemical composition, and physical morphology of PLA-based implants, devices, or scaffolds [58, 59].”
Recent advances and challenges in thermal stability of PVA‐based film: A review
Suleiman, G. S. A., Zeng, X., Chakma, R., Wakai, I. Y., & Feng, Y. (2024) · Polymers for Advanced Technologies · doi:10.1002/pat.6327 · Cited by 111 · cited 1×
“Polyvinyl alcohol is classified as a synthetic polyhydroxy polymer known for its high hydrophilicity, processability, excellent chemical resistance, and biocompatibility [72].”
Yao, X., Yang, X., Lu, Y., Qiu, Y., & Zeng, Q. (2024) · Polymers · doi:10.3390/polym17010066 · Cited by 108 · cited 1×
“This enzymatic action leads to the gradual break-down of polymer into smaller fragments that will be naturally metabolised or excreted by the body [42].”
Factors affecting hydrolysis of polyvinyl acetate to polyvinyl alcohol
Aruldass, S., Mathivanan, V., Mohamed, A. R., & Tye, C. T. (2019) · Journal of environmental chemical engineering · doi:10.1016/j.jece.2019.103238 · Cited by 104 · cited 1×
“…rate of PVA degradation can be influenced by several factors such as its physical form, crystallinity, porosity, molecular weight, degree of hydrolysis, etc. Partially hydrolysed and less crystalline PVA tend to degrade faster due to increased water permeability and reduced hydrogen bonding [82].”
A critical review of fibrous polyurethane-based vascular tissue engineering scaffolds
Fathi‐karkan, S., Banimohamad‐Shotorbani, B., Saghati, S., Rahbarghazi, R., & Davaran, S. (2022) · Journal of Biological Engineering · doi:10.1186/s13036-022-00286-9 · Cited by 104
Recent Advancements in Polyurethane-based Tissue Engineering
Singh, S., Paswan, K. K., Kumar, A., Gupta, V., Sonker, M., Khan, M. A., Kumar, A., & Shreyash, N. (2023) · ACS Applied Bio Materials · doi:10.1021/acsabm.2c00788 · Cited by 104
Complicity of degradable polymers in health-care applications
Anju, S., Prajitha, N., Sukanya, V. S., & Mohanan, P. V. (2020) · Materials Today Chemistry · doi:10.1016/j.mtchem.2019.100236 · Cited by 101 · cited 2×
“As a result, oxidative degradation becomes a biologically regulated process, influenced not only by polymer chemistry but also by immune cell phenotype, activation state, and tissue-specific inflammatory dynamics [43, 44].”
Advances of naturally derived biomedical polymers in tissue engineering
Hu, T., Fang, J., Shen, Y., Li, M., Wang, B., Xu, Z., & Hu, W. (2024) · Frontiers in Chemistry · doi:10.3389/fchem.2024.1469183 · Cited by 99
Filimon, A., Dobos, A. M., Onofrei, M. D., & Serbezeanu, D. (2025) · Polymers · doi:10.3390/polym17081016 · Cited by 99 · cited 1×
“The synthesis of PVA involves the hydrolysis of polyvinyl acetate monomers either through fully or partially hydrolysis procedures [75].”
Polymer Design and Development
Arakawa, C. K., & DeForest, C. A. (2017) · Elsevier eBooks · doi:10.1016/b978-0-12-802734-9.00019-6 · Cited by 94 · cited 1×
“The surface erosion is common in enzymatic-mediated degradation, as enzymes act primarily at polymer surfaces [104, 105].”
Comprehensive review on enzymatic polymer degradation: A sustainable solution for plastics
Suresh, V., Shams, R., Dash, K. K., Shaikh, A. M., & Kovács, B. (2025) · Journal of Agriculture and Food Research · doi:10.1016/j.jafr.2025.101788 · Cited by 94 · cited 1×
“The enzymatic-mediated degradation of PCL occurs through the cleavage of ester bonds in the polymer backbone by specific enzymes, particularly lipases and esterases [93, 102].”
Cutinase-Catalyzed Polyester-Polyurethane Degradation: Elucidation of the Hydrolysis Mechanism
Bisceglie, F. D., Quartinello, F., Vielnascher, R., Guebitz, G. M., & Pellis, A. (2022) · Polymers · doi:10.3390/polym14030411 · Cited by 92 · cited 1×
“The hard segments, typically composed of urethane or urea groups formed from biocompatible diisocyanates, are more resistant but can also be degraded slowly under prolonged enzymatic exposure [127, 128].”
Khan, I., Nagarjuna, R., Dutta, J. R., & Ganesan, R. (2019) · ACS Omega · doi:10.1021/acsomega.8b02642 · Cited by 89 · cited 1×
“The surface erosion is common in enzymatic-mediated degradation, as enzymes act primarily at polymer surfaces [104, 105].”
Effect of Polymer Properties on the Biodegradation of Polyurethane Microplastics
Pfohl, P. M., Bahl, D., Rückel, M., Wagner, M., Meyer, L., Bolduan, P., Battagliarin, G., Hüffer, T., Zumstein, M., Hofmann, T., et al. (2022) · Environmental Science & Technology · doi:10.1021/acs.est.2c05602 · Cited by 85 · cited 1×
“The rate and extent of oxidative degradation depend on the chemical composition of PU, whether it contains aliphatic and/or aromatic biocompatible diisocyanates [133].”
Zhou, J., Fang, C., Rong, C., Luo, T., Liu, J., & Zhang, K. (2023) · Smart Materials in Medicine · doi:10.1016/j.smaim.2023.01.004 · Cited by 85 · cited 2×
“As a result, oxidative degradation becomes a biologically regulated process, influenced not only by polymer chemistry but also by immune cell phenotype, activation state, and tissue-specific inflammatory dynamics [43, 44].”
Åkerlund, E., Diez-Escudero, A., Grzeszczak, A., & Persson, C. (2022) · Polymers · doi:10.3390/polym14163305 · Cited by 80 · cited 1×
“[111], cylindrical PCL filaments showed negligible degradation, 0.6% in 28 days.”
InfluentialYanar, F., Carugo, D., & Zhang, X. (2023) · Molecules · doi:10.3390/molecules28155694 · Cited by 80 · cited 1×
“Polycaprolactone can be processed through various fabrication techniques, such as electrospinning, 3D printing, and solvent casting, that is often combined with other polymers or compounds to enhance its biological performances [97, 98].”
Elgharbawy, A. S., Demerdash, A. G. M. E., Sadik, W. A., Kasaby, M. A., Lotfy, A. H., & Osman, A. I. (2024) · Polymers · doi:10.3390/polym16152141 · Cited by 79 · cited 1×
“This polymer is often chemically modified or blended with more labile and hydrolytically degradable polymers to improve its hydrolytic degradation for TE applications [80].”
Material matters: exploring the interplay between natural biomaterials and host immune system
Tripathi, A. S., Zaki, M. E. A., Al‐Hussain, S. A., Dubey, B. K., Singh, P., Rind, L., & Yadav, R. K. (2023) · Frontiers in Immunology · doi:10.3389/fimmu.2023.1269960 · Cited by 78 · cited 1×
“The desired scaffold materials must exhibit excellent features of biocompatibility, biofunctionality, tolerable biodegradation, adequate strength, and extremely low immunological reaction [23].”
A Review on Polymers for Biomedical Applications on Hard and Soft Tissues and Prosthetic Limbs
Ornaghi, H. L., Monticeli, F. M., & Agnol, L. D. (2023) · Polymers · doi:10.3390/polym15194034 · Cited by 74
Tsai, M.-C., Hung, K., Hung, S., & Hsu, S. (2014) · Colloids and Surfaces B Biointerfaces · doi:10.1016/j.colsurfb.2014.11.003 · Cited by 72
An overview on polyurethane-degrading enzymes
Raczyńska, A., Góra, A., & André, I. (2024) · Biotechnology Advances · doi:10.1016/j.biotechadv.2024.108439 · Cited by 71 · cited 1×
“The soft segments of PU, especially those derived from aliphatic polyesters, are prone to enzymatic attack due to their flexible, accessible structure, and the presence of ester groups [126].”
A road map on synthetic strategies and applications of biodegradable polymers
Meghana, M. C., Nandhini, C., Benny, L., George, L., & Varghese, A. (2022) · Polymer Bulletin · doi:10.1007/s00289-022-04565-9 · Cited by 70 · cited 2×
“These include chemical properties (e.g., composition and surface functionality), structural features (e.g., morphology, porosity, and pore size distribution), and physical characteristics (e.g., crystallinity and wettability) [27].”
Novel drug delivery systems: Insight into self-powered and nano-enabled drug delivery systems
Ewii, U. E., Onugwu, A. L., Nwokpor, V. C., Akpaso, I.-A., Ogbulie, T. E., Aharanwa, B., Chijioke, C., Verla, N., Iheme, C. I., Ujowundu, C. O., et al. (2024) · Nano TransMed · doi:10.1016/j.ntm.2024.100042 · Cited by 68 · cited 1×
“The kinetics of bond cleavage are directly correlated to the type of bonds present in a particular polymeric chain [35, 36].”
Qiu, J., Zhao, H., Luan, S., Wang, L., & Shi, H. (2025) · Biomaterials Science · doi:10.1039/d5bm00122f · Cited by 67 · cited 1×
“Its elasticity and structural integrity make it dominant to be used as scaffolds, vascular grafts, and wound healing materials, where mechanical resilience and gradual resorption are essential [122, 123].”
Groth, T., Stegmayr, B. G., Ash, S. R., Kuchinka, J., Wieringa, F. P., Fissell, W. H., & Roy, S. (2022) · Artificial Organs · doi:10.1111/aor.14396 · Cited by 66 · cited 1×
“…(e.g., the implantation of synthetic prostheses/substitutes to replace failed organs and the utilisation of mechanical devices to assist organ functionalities) have improved patients’ condition, the patients require toleration with subsequence procedures to resume their normal daily life [4–6].”
Lan, W., Zhang, X., Xu, M., Zhao, L., Huang, D., Wei, X., & Chen, W. (2019) · RSC Advances · doi:10.1039/c9ra08569f · Cited by 64
Bahraminasab, M., Doostmohammadi, N., Talebi, A., Arab, S., Alizadeh, A., Ghanbari, A., & Salati, A. (2022) · BioMedical Engineering OnLine · doi:10.1186/s12938-022-01056-w · Cited by 64 · cited 1×
“In another study, PLA that has been printed into 3D scaffolds, has degraded ~4–8% in simulated body fluid (SBF) at 12 weeks [68].”
Du, B., Yin, H., Chen, Y., Lin, W., Wang, Y., Zhao, D., Wang, G., He, X., Li, J., Li, Z., et al. (2020) · Journal of Materials Chemistry B · doi:10.1039/d0tb00656d · Cited by 63 · cited 1×
“For PU-injected moulding films, a moderate degradation of 10–13% was observed at 10 weeks [139].”
Crystallization Study and Comparative in Vitro–in Vivo Hydrolysis of PLA Reinforcement Ligament
Beslikas, T., Gigis, I., Goulios, V., Christoforides, J., Papageorgiou, G. Z., & Bikiaris, D. N. (2011) · International Journal of Molecular Sciences · doi:10.3390/ijms12106597 · Cited by 60 · cited 1×
“The low molecular weight of PLA contributes to facile biodegradation [53].”
Mawad, D., Martens, P. J., Odell, R. A., & Poole-Warren, L. A. (2006) · Biomaterials · doi:10.1016/j.biomaterials.2006.10.007 · Cited by 55 · cited 1×
“[90] have cured 83% and 98% hydrolysed PVA hydrogels with UV and both underwent 100% degradation in PBS at 70 days and 130 days, respectively.”
Sachan, R., Warkar, S. G., & Purwar, R. (2022) · Polymer-Plastics Technology and Materials · doi:10.1080/25740881.2022.2113890 · Cited by 55 · cited 1×
“The existence of ester linkages between carboxyl and hydroxyl groups in the PCL polymeric chain renders its semicrystalline and hydrophobic nature, further tailoring its biodegradability [94].”
Degradation assessment of Mg-Incorporated 3D printed PLA scaffolds for biomedical applications
Ali, F., Kalva, S. N., Mroué, K. H., Keyan, K. S., Tong, Y., Khan, O. M., & Koç, M. (2023) · Bioprinting · doi:10.1016/j.bprint.2023.e00302 · Cited by 55 · cited 1×
“Similarly, 3D-printed PLA scaffolds degraded in phosphate buffer saline (PBS) over 4 weeks exhibited a baseline degradation of approximately 0–1%, which increased to 2–3% upon the incorporation of 15 wt% magnesium AZ61 alloy [63].”
The bio-distribution, clearance pathways, and toxicity mechanisms of ambient ultrafine particles
Han, D., Chen, R., Kan, H., & Xu, Y. (2023) · Eco-Environment & Health · doi:10.1016/j.eehl.2023.06.001 · Cited by 54 · cited 1×
“If the degradation produces insoluble or particulate by-products, the immune sys-tem will be responsible for uptake and clearance through the phagocytic actions of macrophages and neutrophils, such as the by-products of graphene and carbon nanotubes (CNT) [145].”
Enzymatic degradation study of PLA-based composite scaffolds
Donate, R., Monzón, M., Alemán‐Domínguez, M. E., & Ortega, Z. (2020) · REVIEWS ON ADVANCED MATERIALS SCIENCE · doi:10.1515/rams-2020-0005 · Cited by 51 · cited 1×
“For instance, PLA-extruded filaments which possessed 57 ± 2% porosity percentage and 476 ± 52 pore size have degraded 17.6% in Tris–HCl buffer solution containing 0.2 mg/mL of proteinase K and 0.2 mg/mL of sodium azide at 10 days [62].”
InfluentialBiomimetic polyvinyl alcohol/type II collagen hydrogels for cartilage tissue engineering
Lan, W., Xu, M., Zhang, X., Zhao, L., Huang, D., Wei, X., & Chen, W. (2020) · Journal of Biomaterials Science Polymer Edition · doi:10.1080/09205063.2020.1747184 · Cited by 49
Use of Polyesters in Fused Deposition Modeling for Biomedical Applications
Grivet‐Brancot, A., Boffito, M., & Ciardelli, G. (2022) · Macromolecular Bioscience · doi:10.1002/mabi.202200039 · Cited by 47 · cited 1×
“The kinetics of bond cleavage are directly correlated to the type of bonds present in a particular polymeric chain [35, 36].”
Polycaprolactone for Hard Tissue Regeneration: Scaffold Design and In Vivo Implications
Ramírez-Ruiz, F., Núñez‐Tapia, I., Barba, M. C. P., Álvarez-Pérez, M. A., Guarino, V., & Serrano‐Bello, J. (2025) · Bioengineering · doi:10.3390/bioengineering12010046 · Cited by 47 · cited 1×
“Polycaprolactone can be processed through various fabrication techniques, such as electrospinning, 3D printing, and solvent casting, that is often combined with other polymers or compounds to enhance its biological performances [97, 98].”
Wu, H., Yue, L., Jiang, S., Lu, Y. Q., Wu, Y., & Wan, Z. Y. (2019) · Water Science & Technology · doi:10.2166/wst.2019.202 · Cited by 46 · cited 1×
“Subsequently, the carbon–carbon bonds are broken, producing smaller alcohol-based fragments (e.g., vinyl alcohol monomers) or oxidised products (e.g., acetaldehyde or acetic acid) [78].”
Liu, Y.-Y., Blázquez, J. P. F., Yin, G.-Z., Wang, D.-Y., Llorca, J., & Echeverry-Rendón, M. (2023) · arXiv · doi:10.48550/arxiv.2308.15503 · Cited by 46 · cited 1×
“In the previous study, cast PCL films exhibited significantly higher degradation of 20–30% within 23 days [109].”
Biodegradation of Poly(ε-caprolactone): Microorganisms, Enzymes, and Mechanisms
Krumov, N., Atanasova, N., Boyadzhieva, I., Petrov, K. K., & Petrova, P. M. (2025) · International Journal of Molecular Sciences · doi:10.3390/ijms26125826 · Cited by 46 · cited 1×
“Unlike slow hydrolytic degradation, enzymatic-mediated degradation may act robustly, especially in a biological environment where enzymes are present [103].”
Shen, J. J., Yuan, W., Badv, M., Moshaverinia, A., & Weiss, P. S. (2023) · ACS Materials Au · doi:10.1021/acsmaterialsau.3c00027 · Cited by 45 · cited 1×
“While highly hydrophobic electrospun nanofibres with contact angle of 133 ± 1.3°, the degradation remained minimal (0–3% over 12 weeks) [115].”
InfluentialKałużyński, K., Pretula, J., Lewiński, P., Kaźmierski, S., & Penczek, S. (2022) · Macromolecules · doi:10.1021/acs.macromol.1c02325 · Cited by 41 · cited 1×
“The polymerisation of ε-caprolactone monomers is typically initiated by metal cata-lysts such as stannous octoate (Sn(Oct) 2 ) in the presence of an alcohol initiator [99].”
Allan, D., Daly, J. H., & Liggat, J. J. (2018) · Polymer Degradation and Stability · doi:10.1016/j.polymdegradstab.2018.12.027 · Cited by 40 · cited 1×
“The functional groups in PU that are most susceptible to oxidative attack include ether, urethane, and aromatic segments [129, 130].”
Infections after organ transplantation and immune response
Elalouf, A. (2023) · Transplant Immunology · doi:10.1016/j.trim.2023.101798 · Cited by 40 · cited 1×
“Furthermore, these procedures are accompanied by common post-operative issues such as tissue toxicity, immune rejection, inflammation, and bacterial infection [7–9].”
Zuidema, J., van Minnen, B., Span, M. M., Hissink, C. E., van Kooten, T. G., & Bos, R. R. M. (2008) · Journal of Biomedical Materials Research Part A · doi:10.1002/jbm.a.32154 · Cited by 39 · cited 1×
“Polyurethane foams degraded much more slowly, with a reported degradation of 80% over a span of three years [137].”
Brito, J., Andrianov, A. K., & Sukhishvili, S. A. (2022) · ACS Applied Bio Materials · doi:10.1021/acsabm.2c00694 · Cited by 38 · cited 1×
“This is due to the less accessibility of water to the hydrolytically unstable ester linkages found in the polymer backbone [61].”
Wang, B., Ye, X., Chen, G. L., Zhang, Y., Zeng, Z., Liu, C., Tan, Z., & Jie, X. (2024) · Frontiers in Bioengineering and Biotechnology · doi:10.3389/fbioe.2024.1273541 · Cited by 38
Acceleration of Electrospun PLA Degradation by Addition of Gelatin
Bogdanova, A., Pavlova, E. R., Polyanskaya, A., Volkova, M. V., Biryukova, E., Filkov, G. I., Trofimenko, A. V., Durymanov, M. O., Klinov, D. V., & Bagrov, D. V. (2023) · International Journal of Molecular Sciences · doi:10.3390/ijms24043535 · Cited by 37 · cited 1×
“While an extensive study on nanofibre formation by Bogdanova et al. [71] demonstrated that electrospun PLA nanofibres (diameter of 550 ± 300 nm) have degraded ~ 7–9% over 8 weeks immersion in Fenton’s reagent in vitro.”
Lipovka, A. A., Rodriguez, R. D. D., Больбасов, Е. Н., Maryin, P. V., Tverdokhlebov, S. I., & Sheremet, E. S. (2020) · Surface and Coatings Technology · doi:10.1016/j.surfcoat.2020.125560 · Cited by 32 · cited 1×
“Generally, for efficient and tolerable biodegradation, synthetic polymers must have both hydrophobic and hydrophilic moieties, along with amorphous regions in their structure [38].”
Flamini, M. D., Lima, T. A., Corkum, K., Alvarez, N. J., & Beachley, V. Z. (2022) · Materials Advances · doi:10.1039/d1ma01183a · Cited by 32 · cited 1×
“Crystallinity is another critical factor where dense crystalline lamellae have low free volume that reduce the polymer’s chain mobility, thus limiting water absorption and enzyme access [106, 107], while amorphous regions are more readily available for hydrolysation and enzyme penetration.”
Synthesis of Modified Poly(vinyl Alcohol)s and Their Degradation Using an Enzymatic Cascade
von Haugwitz, G., Donnelly, K., Filippo, M. D., Breite, D., Phippard, M., Schulze, A., Wei, R., Baumann, M., & Bornscheuer, U. T. (2023) · Angewandte Chemie International Edition · doi:10.1002/anie.202216962 · Cited by 32 · cited 1×
“The biological degradation of PVA is a random series split of PVA backbone that includes 1,3-glycol structure of two sequential repeating units by a random oxidative dehydrogenation reaction, stimulated by an extracellular secondary alcohol oxidase enzyme [77].”
Fabrication, characterization and evaluating properties of 3D printed PLA-Mn scaffolds
Dehghan-Toranposhti, S., Bakhshi, R., Alizadeh, R., & Bohlouli, M. (2024) · Scientific Reports · doi:10.1038/s41598-024-67478-9 · Cited by 31 · cited 1×
“Dehghan-Toranposhti et al. [66] have printed 3D PLA scaffolds with an initial strut-to-strut spacing of 842 µm and surface wettability of 94.1°.”
InfluentialChen, Y., Etxabide, A., Seyfoddin, A., & Ramezani, M. (2023) · Materials Today Proceedings · doi:10.1016/j.matpr.2023.02.303 · Cited by 28
Bazgir, M., Saeinasab, M., Zhang, W., Zhang, X., Tsui, K. M., Sarvestani, A. M., Nawaz, S., Coates, P. D., Youseffi, M., Elíes, J., et al. (2022) · Journal of Functional Biomaterials · doi:10.3390/jfb13040282 · Cited by 27 · cited 1×
“Biocompatibility involves the favourable interaction of biomaterials with the cellular environment without or with minimum complications, such as inflammation, toxicity, mutagenicity, carcinogenicity, or antigenicity [24].”
Self-citationIn vitro and in vivo degradation correlations for polyurethane foams with tunable degradation rates
Vakil, A. U., Petryk, N. M., Du, C., Howes, B., Stinfort, D., Serinelli, S., Gitto, L., Ramezani, M., Beaman, H. T., & Monroe, M. B. B. (2023) · Journal of Biomedical Materials Research Part A · doi:10.1002/jbm.a.37504 · Cited by 27 · cited 1×
“[143] produced PU-moulded foams with a large pore size of 1100 ± 300 µm that exhibited different degradation behaviours in vitro and in vivo.”
Nabipour, M., Mellati, A., Abasi, M., Barough, S. E., Karimizade, A., Banikarimi, S. P., & Hasanzadeh, E. (2024) · Journal of Biological Engineering · doi:10.1186/s13036-024-00412-9 · Cited by 26 · cited 1×
“[142], electrospun PU with hydrophobicity of 107.6 ± 0.6° had a weight loss of ~ 3% after 8 weeks.”
InfluentialDegradability of Polyurethanes and Their Blends with Polylactide, Chitosan and Starch
Brzeska, J., Tercjak, A., Sikorska, W., Mendrek, B., Kowalczuk, M. M., & Rutkowska, M. (2021) · Polymers · doi:10.3390/polym13081202 · Cited by 25 · cited 1×
“However, the pH-dependent degradation mechanism is not effectively a role in degrading PU as much as PLA since the degradation products of PU are weak carboxylic acids that can be buffered by physiological fluids [134].”
In vivo degradation of poly (ε-caprolactone) films in Gastro Intestinal (GI) tract
Chang, H., Huang, C., Parasuraman, V., Jhu, J.-J., Tsai, C.-Y., Chao, H.-Y., Lee, Y.-L., & Tsai, H. (2017) · Materials Today Communications · doi:10.1016/j.mtcomm.2017.01.006 · Cited by 24 · cited 2×
“In the human body, macrophages (i.e. a type of white blood cell) will subsequently initiate intracellular degradation through the process of phagocytosis where polymer fragments or residues known as foreign subjects are engulfed and internalised into phagosomes [101].”
Stimuli‐accelerated polymeric drug delivery systems
Rust, T., Jung, D., Langer, K., & Kuckling, D. (2022) · Polymer International · doi:10.1002/pi.6474 · Cited by 23 · cited 1×
“For example, poly(ortho esters) and certain polyes-ters degrade more rapidly under acidic conditions due to proton-catalysed cleavage of their backbone bonds [48].”
Dorkhani, E., Faryabi, A., Noorafkan, Y., Heirani‐Tabasi, A., Behboudi, B., Fazeli, M. S., Kazemeini, A., Keramati, M. R., Keshvari, A., & Tafti, S. M. A. (2023) · Journal of Applied Biomaterials & Functional Materials · doi:10.1177/22808000231198803 · Cited by 22 · cited 1×
“[89], non-crosslinked freeze-thawed PVA hydrogels showed fast degradation, with a weight loss of ~ 90–100% after only 4 days in PBS.”
Loloei, Y. H., Mehdikhani, M., Askari, V. R., & Kharazi, A. Z. (2024) · Materials Today Chemistry · doi:10.1016/j.mtchem.2024.101956 · Cited by 22 · cited 1×
“Bead-free electrospun nanofibres, characterised by very fine diameters (175 ± 0.95 nm) and high porosity (87.33 ± 3.56%), have degraded 1.35% in 2 weeks [117].”
InfluentialCalais, G. B., Garcia, G., de Moura, C. F., Soares, J. D. M., Lona, L. M. F., Beppu, M. M., Hernández‐Montelongo, J., & Neto, J. B. M. R. (2025) · Frontiers in Bioengineering and Biotechnology · doi:10.3389/fbioe.2024.1509397 · Cited by 22 · cited 2×
“In the condition of prolonged inflammatory responses (i.e. infection and chronic inflammation), polymer’s degradation will be accelerated due to greater sources of ROS [45, 46].”
Artificial lungs––Where are we going with the lung replacement therapy?
Swol, J., Shigemura, N., Ichiba, S., Steinseifer, U., Anraku, M., & Lorusso, R. (2020) · Artificial Organs · doi:10.1111/aor.13801 · Cited by 21
Huang, B., Wang, Y., Vyas, C., & Bártolo, P. (2022) · Advanced Science · doi:10.1002/advs.202203183 · Cited by 21 · cited 2×
“Molecular weight plays a significant role, where lower molecular weight PCL degrades faster due to shorter polymer chains and greater end-group accessibility [106].”
Špírková, M., Serkis, M. (., Poręba, R., Machová, L., Hodan, J., Kredatusová, J., Kubies, D., & Zhigunov, A. (2016) · Polymer Degradation and Stability · doi:10.1016/j.polymdegradstab.2016.01.003 · Cited by 19 · cited 1×
“Polyurethane cast films exhibited slower degradation, with a range of 2.7–5.0% at 12 months, the addition of macrodiols could increase the degradation to approximately 4.64% [135].”
InfluentialMitropoulou, A., Markatos, D. N., Dimopoulos, A., Marazioti, A., Mikelis, C. M., & Mavrilas, D. (2024) · Journal of Materials Science Materials in Medicine · doi:10.1007/s10856-024-06777-z · Cited by 19
Polyvinyl alcohol degradation by Bacillus cereus RA23 from oil sludge sample
Ullah, M., Li, H., Sun, S., Weng, C., Zhang, H., & Zhu, H. (2019) · 3 Biotech · doi:10.1007/s13205-019-1882-6 · Cited by 18 · cited 1×
“Certain microorganisms and enzymes such as oxidase and dehydrogenase are actively catalysing PVA through the reaction with hydroxyl groups on PVA chains, leading to chain scission and degradation [76].”
Mohamadinooripoor, R., Kashanian, S., Moradipour, P., Sajadimajd, S., Arkan, E., Tajehmiri, A., & Rashidi, K. (2022) · Journal of Polymer Research · doi:10.1007/s10965-022-03165-5 · Cited by 18 · cited 1×
“Moreover, electrospun nanofibres containing 60 wt% polyethylene ether (PEE) exhibited a notable increased degradation from 4.97 to 21.04% within 28 days due to improved hydrophilicity [116].”
InfluentialDíaz, E., Aresti, J., & León, J. (2020) · Journal of Reinforced Plastics and Composites · doi:10.1177/0731684420943304 · Cited by 17 · cited 1×
“Magnetic PCL scaffolds fabricated through freeze-drying demonstrated a baseline degradation of 1.8–2.0% at 8 weeks, which raised to 9.5–10% upon the addition of 10 wt% nHA [114].”
InfluentialHandelsman, S., Overbey, J., Chen, K. Y., Lee, J., Haj, D., & Li, Y. (2023) · Cells · doi:10.3390/cells12121609 · Cited by 17 · cited 1×
“Limited availability of donated organs and timeline accessibility, along with post-trans-plant complications, have increased the mortality rate among patients with chronic diseases [1–3].”
Naureen, B., Ang, B. C., Muhamad, F., Haseeb, A. S. M. A., & Basirun, W. J. (2025) · Polymer Engineering and Science · doi:10.1002/pen.27090 · Cited by 16
Tunable Alginate-Polyvinyl Alcohol Bioinks for 3D Printing in Cartilage Tissue Engineering
Aitchison, A. H., Allen, N. B., Mitra, K., Abar, B. M., O’Neill, C. N., Bagheri, K., Anastasio, A. T., & Adams, S. B. (2024) · Gels · doi:10.3390/gels10120829 · Cited by 15 · cited 1×
“Three-dimensional printed bioink scaffolds made of 15% w/v PVA were found degraded by ~ 10% over 28 days in a high glucose cell culture medium [91].”
Vijayaraghavan, K., & Ali‐Seyed, M. (2018) · Annual Research & Review in Biology · doi:10.9734/arrb/2018/39648 · Cited by 14
Sadia, M., Zaki, M. A. M., Jaganathan, S. K., Shakhih, M. F. M., Kamarozaman, A. S., Ab’lah, N. N., & Saidin, S. (2023) · Arabian Journal for Science and Engineering · doi:10.1007/s13369-023-07736-6 · Cited by 14
Self-citationBiodegradation of PLA-Pennisetum purpureum based biocomposite scaffold
Revati, R., Majid, M. S. A., Ridzuan, M. J. M., Normahira, M., Nasir, N. F. M., & Cheng, E. M. (2017) · Journal of Physics Conference Series · doi:10.1088/1742-6596/908/1/012029 · Cited by 13 · cited 1×
“While PLA-casted scaffolds demonstrated much higher degradation in PBS with 20.10% weight loss, which was further increased to 27.4% upon the incorporation of Pennisetum purpureum after 40 days of degradation test [64].”
InfluentialKhoshnood, N., Shahrezaee, M. H., Shahrezayee, M., Shams, A., & Zamanian, A. (2022) · Journal of Applied Polymer Science · doi:10.1002/app.52628 · Cited by 13
Khan, T., Mirza, E. H., Kurd, N. J., Naushad, M., & Haque, M. Z. U. (2023) · Digest Journal of Nanomaterials and Biostructures · doi:10.15251/djnb.2023.183.821 · Cited by 13 · cited 1×
“While PVA freeze-thawed hydrogels immersed in SBF for 5 weeks showed a decline in degradation with the increasing of PVA concentrations; 2% PVA (45% weight loss), 5% PVA (38% weight loss), and 10% PVA (34% weight loss) [92].”
Mechanical Properties of 3D Printed PLA Scaffolds for Bone Regeneration
Kundreckaitė, P., Šešok, A., Stonkus, R., Gaidulis, G., Romańczuk-Ruszuk, E., & Pauk, J. (2024) · Acta Mechanica et Automatica · doi:10.2478/ama-2024-0072 · Cited by 13 · cited 1×
“Longer-term degradation study at 20 weeks revealed that PLA scaffolds immersed in PBS exhibited approximately 10% weight loss [69].”
Ahmed, S., Pfeiffer, R. M., Volesky, K. D., Blosser, C. D., Snyder, J. J., Israni, A. K., Lynch, C. F., Qiao, B., Rees, J. R., Zwald, F. O., et al. (2025) · American Journal of Transplantation · doi:10.1016/j.ajt.2025.03.004 · Cited by 13
Jumat, M. A., Chevallier, P., Mantovani, D., Copes, F., Razak, S. I. A., & Saidin, S. (2021) · Polymer-Plastics Technology and Materials · doi:10.1080/25740881.2021.1876879 · Cited by 12 · cited 2×
“It can be tuned by altering the stereochemistry, chemical composition, and physical morphology of PLA-based implants, devices, or scaffolds [58, 59].”
Self-citationToxic effects of heavy metal exposure in solid organ transplant recipients
Glicklich, D. G., Mustafa, M., & Wolfe, K. (2024) · Transplantation Reports · doi:10.1016/j.tpr.2024.100151 · Cited by 9
Cancer mortality among solid organ transplant recipients: A systematic review and meta-analysis
Wang, Z., Deng, L., Hou, W., Liu, S., Zhang, Y., Sheng, C., Zhang, Y. L., Li, J., & Shen, Z.-Y. (2024) · Preventive Medicine · doi:10.1016/j.ypmed.2024.108161 · Cited by 8
Ambreen, J., Malick, T. P., Tan, J. F., Zulfikree, H. S., Gopal, R., Kim, H. Y., Sivalingam, S., Ali, H., & Saidin, S. (2024) · Journal of Drug Delivery Science and Technology · doi:10.1016/j.jddst.2024.106221 · Cited by 5 · cited 2×
“Another PU electrospun membrane, with nanofibre diameter of 0.87 ± 0.06 µm, showed a higher degradation range of 15–18% after 60 days, which increased to 18–30% when chitosan and elastin were added [20].”
InfluentialSelf-citationSelvaras, T., Jaganathan, S. K., Sivalingam, S., & Saidin, S. (2022) · Journal of Human Centered Technology · doi:10.11113/humentech.v1n1.8 · Cited by 3 · cited 1×
“[140] showed that electrospun PU fibres loaded with chitosan nanoparticles showed a mild increase in degradation from 3–4% to 4–5% over 60 days.”
Self-citationWattanutchariya, W., & Suttiat, K. (2022) · Chiang Mai University Journal of Natural Sciences · doi:10.12982/cmujns.2022.008 · Cited by 2 · cited 1×
“Wattanutchariya and Suttiat [67] demonstrated PLA-casted films (wettability of 69.43 ± 0.42°) exhibited a degradation range of ~3–6% after PBS immersion for 90 days.”
InfluentialKhrisna, D. F., Ambreen, J., Wei, T. Y., Riduan, N. A. H., Daud, N. M., Zain, N. M., Abdullah, F., Malek, N. A. N. N., Ulum, M. F., & Saidin, S. (2025) · Journal of Biomedical Materials Research Part B Applied Biomaterials · doi:10.1002/jbm.b.35575 · Cited by 2 · cited 2×
“[108] showed that electrospun PCL nanofibres with fibre diameter of 1.73 ± 0.35 μm and porosity of 27.09 ± 4.07% have produced 2.5–3.0% degradation at 60 days of analysis due to their inherent hydrophobicity (115.03 ± 3.69°).”
InfluentialSelf-citationTarmizi, Z. I. A., Ali, R. R., Nasef, M. M., Radzi, A. M. M., Akim, A. M., Eshak, Z., Noor, S. M., Shafie, N. F. A., & Faizo, S. M. (2023) · Journal of Advanced Research in Fluid Mechanics and Thermal Sciences · doi:10.37934/arfmts.108.2.110121 · Cited by 1 · cited 1×
“[138] described electrospun PU-grafted with 2-hydroxyethyl methacrylate (HEMA) showed a much slower degradation, with weight loss reduced to 0.5–1.5% compared to the initial PU degradation of 13–15% at 84 days.”
InfluentialFabrication and Characterization of Pla-Based Biopolymer Composite for Biomedical ApplicationsPreprint
Rahman, M. M., Ali, O., Ali, M. R., Islam, M. A., Mahmud, S., Khatun, H., & Ali, Y. M. (2024) · SSRN Electronic Journal · doi:10.2139/ssrn.4942467 · Cited by 1
Research works printed but not linked: 2
- Saidin S, Muhamad Zain N, Mohd Daud N. Polymeric materials for drug delivery: insight into biomedical applications. 1st ed. Johor Bahru: Penerbit UTM Press; 2025.
- Selvaras T, Ali Alshamrani S, Gopal R, Jaganathan SK, Sivalingam S, Kadiman S, et al. Biodegradable and antithrombogenic chitosan/elastin blended polyurethane electrospun membrane for vascular tissue integration. J Biomed Mater Res B Appl Biomater. 2023;111:1171–81. https://doi.org/10.1002/jbm.b.35. · doi:10.1002/jbm.b.35
Cited by
Portan, D. V., Kontaxis, L. C., Tselepidi, A., Papanicolaou, G. C., & Azamfirei, L. (2026) · Polymers · doi:10.3390/polym18161984 · Cited by 2
“With prolonged exposure, these processes may lead to loss of polymer integrity, surface erosion, fragmentation, and eventual mass reduction [28,29].”
Di, J., He, Y., Sun, C., Jia, J., Zheng, X., & Li, X. (2026) · Gels · doi:10.3390/gels12060498
“[48–54] Biofunctionalization, through the grafting of anti-inflammatory factors and growth factors, provides the overarching direction for cell recruitment, inflammation suppression, and oriented differentiation in cartilage regeneration.”
Deng, W., Liu, Y., Zhong, Y., Wang, J., & Zhang, J. (2026) · International Journal of Nanomedicine · doi:10.2147/ijn.s625193
“59 ③ Protein-based materials, such as gelatin and collagen—for example, collagen hydrogels derived from porcine skin have shown controllable drug-release properties because of their transparency and rigidity 60 —and silk fibroin, 61 which can be structurally modified to prepare functional hydrogels…”
Demirci, G., Niedźwiedź, M., Kordek, W., Charęza, M., Drozd, R., & Fray, M. E. (2026) · European Polymer Journal · doi:10.1016/j.eurpolymj.2026.115175
Inside-out and monitoring-assisted phototheranostics enabled by molecular–optoelectronic integration
Xu, G., Zhong, Y., Zhang, Y., Law, W., & Xu, Z. (2026) · Coordination Chemistry Reviews · doi:10.1016/j.ccr.2026.218424
Metadata
- Authors
- Saidin, S., Zubairi, S. I., Ambreen, J., Md Lazim, N. A., Sadia, M., Lim, J. T. W., Ulum, M. F., Elliyanti, A., & Sefat, F.
- Affiliations
- University of Technology Malaysia (MY)
- National University of Malaysia (MY)
- COMSATS University Islamabad (PK)
- NED University of Engineering and Technology (PK)
- Newcastle University (GB)
- IPB University (ID)
- Andalas University (ID)
- University of Bradford (GB)
- Corresponding author
- Saidin, Syafiqah
- ORCID
- Venue
- BioMedical Engineering OnLine
- Published
- 2026-05-05
- Volume
- 25
- Issue
- 1
- ISSN
- 1475-925X (ISSN-L)
- PMC
- PMC13289440
- OpenAlex
- W7160285667
- Cited by
- 8
- References
- 142
- Citations by year
- 2026: 8
- FWCI
- 3.51
- Type
- journal article
- Language
- en
- Open access
- gold
- doi.org
- Licence
- cc-by
- creativecommons.org/licenses/by/4.0 (tdm)
- creativecommons.org/licenses/by/4.0 (vor, 49 d)
- Locations
- BioMedical Engineering OnLine (publishedVersion, cc-by)
- PubMed (publishedVersion)
- PubMed Central (publishedVersion, cc-by)
- DOAJ (DOAJ: Directory of Open Access Journals) (submittedVersion)
- Funders
- Department of Deputy Vice Chancellor (Research & Innovation), Universiti Teknologi Malaysia (Q.J130000.4609.00Q10)
- Topics
- Physical Sciences › Materials Science › Biomaterials › biodegradable polymer synthesis and properties
- Physical Sciences › Materials Science › Biomaterials › Hydrogels: synthesis, properties, applications
- Health Sciences › Medicine › Surgery › Surgical Sutures and Adhesives
- Keywords
- polymer degradation kinetics, tissue engineering scaffolds, polylactic acid, polyvinyl alcohol, polycaprolactone, polyurethane, hydrolytic degradation, enzymatic degradation, oxidative degradation, pH-dependent degradation, load-bearing implants
- MeSH terms
- Animals, Biocompatible Materials, Humans, Kinetics, Polymers, Regeneration, Tissue Engineering
About these checks
Registry, retraction, Cites and statistics results are computed, not judged, with one exception: a printed reference that no index lists is read once by a model before it counts as a citation error. Claims are extracted by a model and kept only when their quote appears verbatim in the text; each cited source is then checked, with a model’s help, for whether it says what the claim relies on. Those verdicts can be wrong — read the claim’s quote and the cited source before relying on one.
A language model drew the claims from the paper on 2026-10-11, under version 3 of the claim definition (model deepseek-v4.1-flash, prompt extract-v3).
A second model labelled each claim on 2026-10-11 (model jev-1.13-20260917, definition revision gold-guideline-v0.2).
Statistics and arithmetic are recomputed, not judged.
Confidence bands are shown only for fields calibrated on our annotated test set. None is calibrated yet, so no band is shown.
What counts as a claim ›How we measure confidence ›How we check this ›
Are you an author, or do you see a problem with this page? Request a review
Data sources
Bibliographic data: Semantic Scholar, OpenAlex, Crossref.
Contains information from the Semantic Scholar Academic Graph Datasets, made available under the ODC Attribution License (ODC-BY 1.0).
Semantic Scholar’s data is described in: Kinney, R., et al. (2023). The Semantic Scholar Open Data Platform. arXiv:2301.10140.